- 1StrengthMax stress before yield/fracture
- 2StiffnessResistance to deformation elastically
- 3DuctilityAbility to plastically deform significantly before rupture
- 4ToughnessEnergy absorbed before fracture (Tensile/Impact/Fracture)
Energy absorbed before yield (Modulus of resilience) - 5HardnessResistance to permanent deformation (scratch, dent)
- 6Fatigue ResistanceResistance to fracture under cyclic load
- 7Creep ResistanceResistance to plastic deformation under long-term stress
- 8Yield StrengthThe point where the material transitions from elastic to plastic deformation (obtained from tensile test)
- 9Modulus of ResilienceThe elastic energy a material can absorb prior to yielding
Er = 1/2(yield strength)(strain at yielding) - 10Stress-Strain Curve

- 11Work Hardening Exponent (n)

- 12Ductile vs Brittle Fracture

- 13Temperature Effect on Ductile Metal-Modulus of elasticity: E does not change
-Yield strength: As temp increases, Sy decreases (due to dislocation movement)
-Tensile (ultimate) strength: As temp increases, Sut decreases (due to dislocation density)
-Tensile Toughness: As temp increases, U increases - 14Ductile-Brittle TransitionBCC material transitions from brittle to ductile at this temp
- 15Hardness Measurement TechniquesTesting: Brinell, Rockwell, Microhardness, and nanoindentation
Benefits: inexpensive, nondestructive, can be used to estimate other mechanical properties (tensile strength) - 16Fracture Toughness (Kc)Material property
Stress intensity factor required for crack to propagate
Higher Kc means less crack propagation, more energy absorption
Factors improve Kc - How?
-Ability to deform (ductility). e.g. higher temp
-Potentially smaller grain size? Crack needs more energy to propagate through one grain to next grain
-Lower dislocation density (ductility inc.) - 17Modes of Fracture

- 18Ductile Fracture1. Proceeds relatively slowly
2. Extensive plastic deformation
3. Stable crack
4. Require more strain energy
5. Easier to see the warning
6. Most metals/some polymers (T > Tg)
7. Cup-and-cone fracture surface - 19Brittle Fracture1. Cracks may spread rapidly
2. Little plastic deformation
3. Unstable crack
4. Less strain energy
5. Occurs suddenly without warning
6. Ceramics/some metals/some polymers (T < Tg)
7. Fracture surface perpendicular to the direction of the applied stress
8. Relatively flat, bright, smooth, fracture surface
9. Chevron patterns (V-shaped markings) due to crack propagates from the origin at different levels - 20Weibull StatisticsProbability of fracture vs. applied stress
Brittle fracture uses Weibull Distribution
Any stress > 0 in brittle material is possible to cause fracture
Weibull modulus (m) - slope of Weibull plot
Characteristic Strength (sigma_0) - ln(sigma0) is the x-intercept of Weibull plot - 21FatigueThe lowering of strength of failure of a material due to repetitive stress which may be above or below the yield strength
N - # of cycles to failure
S - typical amplitude of stress (sigma_a) - 22Crack Growth Rate1. Below threshold delK, crack will not grow
delKth = Kop - Kmin
2. Slow growth
3. Power Law
da/dN = C(delK)^n
4. Rapid growth (unstable)
Kmax > KIC - 23Improve Fatigue LifeMost cracks leading to the fatigue failure originate at surface position especially at stress concentration site
-Reduce stress concentration in design
-Surface treatment - 24CreepTime dependent deformation under constant stress (below yield strength, typically at higher temp)
The time required for failure is the rupture time
The creep rate and rupture time (tr) follows an Arrhenius relationship - 25PolymerizationChemically join small molecules (monomer - one unit, or oligomers - a few units) to form giant molecules
- 26Polymer ArchitectureAffect density, strength, viscosity, solubility, glass transition temperature (Tg)
Increasing Strength: Linear, Branched, Cross-Linked, Network - 27ThermoplasticsLinear or branched molecules
Weak Van der Waals between chains
Low Tg and melt (Tm) upon heating
Easy to recycle e.g. Polyethylene (PE) - 28ThermosetsHighly cross-linked or 3D network structure
Stronger but more brittle than thermoplastics
High Tg, decompose at high T (no Tm)
Hard to recycle e.g. Polyurethane (PU) - 29Addition PolymerizationFree radical polymerization
By broken unsaturated double bond (by T, P, catalyst) - 30Condensation PolymerizationA small molecule (water, ethanol, methanol, etc.) forms during condensation polymerization
- 31Degree of PolymerizationNumber of repeat units
(Average molecular weight of polymer) / (Molecular weight of repeat unit) - 32TacticityDistribution or arrangement of non-symmetrical repeat unit (atoms or atomic groups)
-Isotactic: atoms are all on the same side
-Syndiotactic: atoms generally occupy positions on opposite side of chains
-Atactic: random arrangement of atoms (poor packing, low density, low strength, poor resistance to heat or chemical attack) - 33CopolymersContains 2 or more types of monomers

- 34Temperature Effects on PolymersDepends on whether the polymer is easy to crystallize and cooling rate
-Rubbery and leathery state: Tm>T>Tg, under stress => elastic and plastic deformation
-Glassy state: Hard, rigid, brittle, T - 35Crystallinity in PolymersPolymers are never 100% crystalline. They are semicrystalline material consists of crystalline regions and amorphous regions
Crystallinity affect physical, chemical and optical properties
-Higher crystallinity => denser, stiffer, harder, tougher and more resistant to solvents - 36Mechanical Properties of ThermoplasticsMostly non-newtonian, viscoelastic behavior
Elastic behavior:
-Distort segments of polymer chains: Recovery over a long period of time => viscoelastic elastic deformation
-Stretch and distort covalent bonds => elongate chain elastically: Recovery is instantaneous - 37Plastic Deformation of ThermoplasticsStress drop beyond yield pt
Chain will stretch, rotate, slide or disentangle
Necking: continued sliding of the chains in necking region
When chains are nearly parallel:
-van der Waals force lined up
-need greater stress to deform - 38Viscoelastic CreepThermoplastics exhibit creep, a time dependent permanent deformation with constant stress or load
Due to movement of chains (vs. diffusion in metal) - 39Stress RelaxationStress decreases with time at constant strain
Relaxation occurs more rapidly at higher T - 40CrazingOccurs in thermoplastics when localized regions of plastic deformation occur in a direction perpendicular to that of the applied stress
- 41BlushingRefers to failure of a plastic because of localized crystallization (due to repeated bending, for example) that ultimately causes voids to deform
- 42ElastomersCoil like deformation, large elastic deformation > 200%
Can be thermosets or thermoplastics
Prevent viscous plastic deformation while retaining large elastic deformation by cross-linking the chains - 43Cold WorkingThe application of a stress higher than yield strength to a metal, deforming it and increasing strength by leaving a residual strain
Effective in simultaneously shaping and strengthening metals at the expense of reducing ductility
At low T, deform and strengthen the material at same time
Manufacturing Processes: forging-open die, rolling, extrusion, forging-closed die, stamping, wire drawing - 44Strain Hardening Exponent (n)higher n, higher yield strength, work hardening effect is stronger
- 45Strain Rate Sensitivity (m)Describes how the flow stress changes with strain rate
It is useful for predicting high-impact behavior of a material
Typically m < 0.1 for metals and increases with temperature
In general, higher values of m and n can resist necking => better formability - 46SpringbackThe elastic strain that is recovered after a material has been plastically deformed
It is important in the processing of polymers by extrusion and shaping automotive body panels from sheet steel - 47Bauschinger EffectThe effect in which a material which has been plastically deformed under a tensile stress shows a reduction in compressive strength, and vice versa
- 48Strain Hardening MechanismsDuring plastic deformation of metals, dislocations density increases
Eventually dislocations interfere with their own motion, increasing strength - 49Little to No Strain Hardening in Certain Materials-Ceramics
*Can have some small strain hardening
*Dislocations are not very mobile and porosity (Cold working not usually possible)
-Silicon
*Too brittle to strain harden appreciably
-Glasses
*Amorphous => no dislocations => no strain hardening
*residual stress caused by cooling rate difference: Tempered glass (compressive stress)
*Annealed glass (no or little stress) - 50Strengthening in Polymers (Thermoplastics)Strengthen upon deformation
-Alignment and/or crystallization of polymer chains - 51Properties vs. Percent Cold WorkStrain hardening controlled by the amount of plastic deformation, defined by the % CW
% CW inc., yield and tensile strengths inc., ductility dec. - 52Anisotropy From Sheet TextureDuring rolling, grains rotate and elongate, causing certain crystal directions/planes to become aligned in rolling direction
- 53AnnealingCan remove effects of cold working
-Low T: eliminate residual stresses but maintain mech. prop.
-High T: can reverse strain hardening
Three Stages:
1. Recovery (Removes residual stress)
-Thermal energy permits dislocations to move and reduce residual stress
-Form polygonised subgrains
-Dislocation density remains the same (or similar)
-Also called stress-relief annealing
2. Recrystallization (dec. strength, inc. ductility)
-New and small grains form, dislocations vanish
-New grains tend to grow on the dislocation created polygons
-Recrystallization temperature is not a fixed temperature
3. Grain growth (Hall-Petch dec. yield strength)
-Big grains grow by consuming smaller surrounding ones
-Driven by reduction of grain boundaries
-Strength decreases with reduced grain boundaries (big grains) - 54Recrystallization TemperatureTr decreases as % CW increases
Smaller grain size, lower the Tr
Tr of pure metals is lower than that of alloys
Increasing the annealing time reduces Tr
For most of metals (in Kelvin): Tr ~ 0.4Tm
Tr is a boundary between cold and hot working temperatures - 55Hot WorkingPlastically deforming above Tr
Almost unlimited deformation
No strengthening
-Recrystallization simultaneously
Pros:
-easier to shape (less force required)
-eliminate imperfections (eg. dislocations, gas pores)
Pro or Con:
-Anisotropic behavior due to different cool rates
Cons:
-Poor surface finish and dimensional accuracy (oxidation of the surface, difficult to control dimensions) - 56Selection of Materials Processing*Cold Working
-We can increase the maximum deformation of a material by doing a series of cold working and subsequent annealing until the desired dimensions are reached
*Hot Working
-When a material is for high temperature service, recrystallization immediately causes catastrophic decrease in strength
-Too many cycles using cold working - 57NucleationFormation of secondary phase from a primary phase
In solidification: formation of first nanocrystallites from molten metal - 58Critical Radius (r*)Radius above which particle growth is accompanied by a decrease in free energy (spontaneous)
- 59del G*Energy required to form a stable nucleus (i.e. from an infinitely small particle)
- 60Critical Size for NucleationWhen Tm - T increases, r* decreases
Undercooling: Tm - T
del Gv increases, del G* decreases, required less energy to form a stable nucleus - 61Heterogeneous NucleationHeterogeneous nucleate sites:
-Impurities in the liquid
-Wall of container
Less undercooling is needed
r* is the same. To form the curvature of a radius of r*, it requires much less atoms in the nucleus (the spherical cap) - 62Hetero- vs. Homogeneous eneous NucleationHomogeneous needs large undercooling to form stable nuclei
*Almost never occurs in liquids
Heterogeneous requires less undercooling
*On preexisting surfaces (e.g. Dust particles, Secondary phase particles, Mold walls and cracks)
r* depends on T (r*hom = r*het)
delG*hom > delG*het
delG*het depends on delT and theta - 63Controlled Nucleation-Inoculation: Adding small particles to promote nucleation => smaller grains and higher strength (e.g. adding Ti, B into Al alloy, forming Al3Ti and TiB2 serve as sites of nucleation
-Dispersion strengthening: Form an ultra precipitates (second phase) through solid state transformations => higher strength
-Metallic glasses: fast cooling to prevent nucleation of crystallization - 64Growth Mechanisms of Planar GrowthThe manner of the growth of solid nuclei depends on how heat is removed
Well-inoculated => heterogeneous nucleation (start from wall/impurities) => no need for undercooling
Temp in liquid ahead of front is greater than Tm
Removes heat from the liquid-solid interface via conduction
-The formation of protuberance decrease temperature difference between interface and nearby solid, heat dissipation is harder, growth slow down
-The remainder of the interface catches up - 65Growth Mechanisms of Dendritic GrowthNot well-inoculated => need undercooling in liquid
Temp in liquid ahead of front is smaller than Tm
Dissipate heat to the liquid ahead
-Proceeds until the liquid is not undercooled any more => planar growth
-Only a small fraction of the total growth in pure metals - 66Solidification Time (Casting)Chvorinov's Rule is a mathematical relationship that relates the solidification time for a simple casting to the volume and surface area
V - Volume of casting (larger volume means more heat to dissipate)
B - Mold constant, depending on casting conditions, e.g., heat of fusion, initial temperatures, heat capacity of mold, etc.
A - Surface area in contact with mold - heat is transferred from the casted material to the mold through this area - 67Secondary Dendrite ArmCooling rate inc., heat dissipating rate Q' inc., finer dendritic network (more efficient conductor of latent heat), Secondary Dendrite Arm Spacing (SDAS) dec.
- 68Cooling CurvesDuring solidification 2 types of heat must be removed:
-latent heat of fusion
-specific heat - 69Casting MicrostructuresMultiple morphologies:
-Columnar grains (anisotropic properties)
-Equiaxed grains (isotropic properties) - 70Solidification Defects - ShrinkageShrinkage (reduction in volume during solidification for most materials)
Interdendritic Shrinkage (Micro-porosity) - 71Solidification Defects - Gas PorositySolubility of gas in molten materials is relatively large
Solubility decreases upon solidifying
-Forms bubbles that can be trapped in solid
To prevent:
-Add materials to liquid that combine with the gas to form a solid
-Ensure the partial pressure of the gas remains low - 72Casting Techniques1. Sand Casting
-Mold: green sand (water/clay/sand) or ceramics
-Problem: cavity
2. Investment Casting
-Ceramic mold coated on wax
-Lost wax process: wax removed for casting
-Pros: complex shape
-Appl: golf club head, bioimplants, turbine blades
3. Permanent Mold Casting
-Pros: Good surface, dimensional accuracy, rapid solidification, high strength, reusability
-Cons: high cost, limited complexity in shapes
4. Pressure Die Casting
-Pros: Smooth, high quality surface, dimensional accuracy
-Cons: high cost - 73Ingot CastingCasting steel in molds; smaller quantity
Non ferrous metals (Zn, Cu) - 74Continuous CastingFrom molten liquid metal directly to semi-finished shape
Cost effective for steels, Al alloys - 75Directional Solidification: Single CrystalConventional - equiaxed grains
-Problems: transverse failure along GBs
Directional - multiple grains with GBs align along growth direction
Single Crystal - even better for turbine blade - 76Joining of Metallic MaterialsBrazing - joining metals with fillers (Tm or filler > 450 C)
Soldering - Tm or filler < 450 C
Characteristics of brazing/soldering
-Metals being joined do not melt
-Filler melt
-Filler material is different from base material
Fusion Welding
-Metals being joined also melt
-Fusion Zone (FZ), Heat Affected Zone (HAZ)
-Fast cooling can help refine grains in FZ
*Arc welding, laser welding, friction stir welding
Información
- Descripción
- Engineering Fichas sobre MEEN 360 Midterm Exam Study, creado por Daniel Varnau el 01/03/2024.
- Creado por
- Daniel Varnau
- Visitas
- 6
- Valoración